Technical report on the investigation of various metal bearing materials, including Hall's metal and white metal alloys.


Identifier  ExFiles\Box 115\1\  scan0142
Date  19th November 1936
  
Cont'd. {John DeLooze - Company Secretary} -2- Rm {William Robotham - Chief Engineer} 6/R.19.11.36.

(1) HALL'S METAL BEARING. BIG ENDS.

have carried out indicates that ordinary RR.56 forged alloy is better than any of the tin aluminium alloys. We feel fairly confident that this bearing will be satisfactory once we get a satisfactory main bearing. We are reassured in this by the fact that Leylands have been running big ends in this material for some considerable time, and are completely satisfied with it.

During our investigations we have been able to improve the lubrication of the big end by alteration to the crankshaft.

(2) HALL'S METAL. MAINS.

With regard to the main bearing in Hall's Metal alloy, the bearing material with the minimum amount of tin, i.e., 1%, shows the most promise on the main bearings. There is no indication whatever that this will be any kinder to the crankshaft than the material which is already in production, and we are not, therefore, contemplating sending this combination to France until we have a harder crankshaft. Such material is available in Hykro, and the necessary forgings are in hand, but it will probably be six weeks or more before we get a crankshaft.

B. WHITE METAL BEARINGS - GENERAL POSITION.

The American Automobile Manufacturers have behaved in much the same way as we have. They found the babbit would not stand, went rather hurriedly into new bearing materials, and are now in full retreat. The majority of them are going back to babbit. The reason they are doing this is because the Babbit people have managed to improve their material considerably. At the present moment, in this country, Hoyt's have produced two improved babbit materials:-

Z.S. This has 3% silver in it, and Bristol's have done a good deal of work on it and are now in production. This gives a certain amount of confidence. Bristol's estimate that it will stand up to about 25% greater loads than anything they have previously had of the same type.

11.H. This is a more experimental material, which contains 4% of cadmium. From Hoyt's results it is able to withstand higher loads and
  
  
From the Rolls-Royce experimental archive: a quarter of a million communications from Rolls-Royce, 1906 to 1960's. Documents from the Sir Henry Royce Memorial Foundation (SHRMF).


Copyright Sustain 2026, All Rights Reserved.    whatever is rightly done, however humble, is noble
An unhandled error has occurred. Reload 🗙