Rolls-Royce Archives
         « Prev  Box Series  Next »        

The performance and wear of Eska Tungsten distributor points after running for 11,587 miles on a 20 HP chassis.


Identifier  ExFiles\Box 35\6\  scan 133
Date  26th June 1924
  
EFC. {E. Fowler Clarke - Electrical Engineer}
EA.52.
26th June, 1924.

ESKA TUNGSTEN POINTS AQ OFF CHASSIS 7-GII.

These points have run altogether 11587 miles on a 20 HP. distributor fitted to 7-GII.

Screw point. About 90% of the surface has been in contact. No appreciable wear in the depth of the point. Worn surface very rough with a rather large cavity at the centre, and badly discoloured.

Lever Point. About 60% of the surface has been in contact. Very little wear in the depth. Surface fair, with a rough projection presumably corresponding with the cavity in the screw point, when both are in position. The general condition of the points can be considered to be only fair; the wear, good.

The tester on the chassis test reports that these points required trimming more frequently than usual, and that the apparent oxidation of the points tended to cause rather worse low speed sparking on the engine than when the points had been trimmed and cleaned. His opinion is that these points are not as good as the platinum (standard).

EFC {E. Fowler Clarke - Electrical Engineer} /HEW.
  
  
From the Rolls-Royce experimental archive: a quarter of a million communications from Rolls-Royce, 1906 to 1960's. Documents from the Sir Henry Royce Memorial Foundation (SHRMF).


Copyright Sustain 2026, All Rights Reserved.    whatever is rightly done, however humble, is noble